1 t/h Coated Aluminium Decoating Line
One tonne an hour suits a fabricator that generates its own painted offcuts, or a dealer who buys coated extrusion from a handful of window makers. Two zones are enough at this rate, and the short tunnel keeps the capital down without compromising the one thing that matters — a single layer of charge and enough dwell to burn the film clean.
Sections the tunnel can take
The range runs from printed foil at 0.05 mm to architectural profile at 4 mm, and the dwell is set by the heaviest section in the batch. Mixing foil into a profile batch is how a tunnel produces both scorched foil and under-burnt profile in the same pass.
| Section | Zone 1 | Zone 2 | Dwell |
|---|---|---|---|
| Foil 0.05–0.2 mm | 430 °C | 470 °C | 4–5 min |
| Sheet 0.5–1.5 mm | 460 °C | 505 °C | 7–10 min |
| Profile 2–4 mm | 490 °C | 525 °C | 12–16 min |
Two zones mean the second one has to do the work of both a burn and a soak on the larger three-zone tunnel. In practice it is set slightly hotter and the belt is run slower, which is why a one-tonne line can hold 0.8–1.8 % metal loss but not the 0.7 % a five-zone tunnel reaches on the same feed.
Line arrangement and drives
| Stage | Function | Power | Key setting |
|---|---|---|---|
| Belt loader and spreader | Single-layer charging, 1.2 m belt | 3 kW | Layer depth below 60 mm |
| Tunnel | Two zones, 8 m heated, mesh belt | 8 kW drives | Burners per zone, 525 °C ceiling |
| Cooling section | Forced air, 3 m | 4 kW | Discharge below 150 °C |
| Off-gas train | Cyclone, afterburner, bag filter | 7 kW | 850 °C, 2 s residence |
| Discharge baler | Bales coated scrap for remelt | 11 kW | Bale 25–40 kg |
The spreader is the cheapest insurance on the line. A bed three sections deep decoats from the outside in, and the operator compensates by raising zone 2 until the outer surfaces oxidise — producing a batch that is scorched outside and still painted in the middle. The spreader costs a few thousand dollars and removes that failure mode entirely.
Footprint and off-gas
Eighteen by four metres including the baler, with 1 m of access on the burner side and 2 m at the discharge. The afterburner and bag filter sit outside against the wall, which keeps the radiant heat out of the working area and shortens the duct run to the stack.
| Service | Requirement | Note |
|---|---|---|
| Electrical | 45 kW installed, 63 kVA supply | Baler is the largest single load |
| Gas | 14–20 m³/h | Two zone burners plus afterburner |
| Compressed air | 6 bar, 0.3 m³/min | Damper and bag-pulse actuation |
| Water | None in process | Washdown tap only |
| Stack | 4 m above ridge | Sample port above the filter |
Consumables and cost per tonne
Gas per tonne is the highest in the coated-aluminium family at this size: the short tunnel has less internal heat recovery, and the afterburner duty is spread over less material. The difference against a five-zone tunnel is around 30 %, which is a real number in a plant running two shifts.
| Item | Value | Notes |
|---|---|---|
| Gas | 38–52 m³/t | Foil at the top of the range |
| Heat recovery | 45–60 % of burner duty | Zone 1 combustion air only |
| Metal loss | 0.8–1.8 % | Thin sections lose most |
| Mesh belt life | 8–14 months | Depends on temperature cycling |
| Crew | 2 per shift | One on charging and zones |
| Capital, indicative | USD 145k–225k | EXW, excluding civils and stack |
Buyer supplies and sizing traps
The buyer provides the floor and the 63 kVA supply, gas and air, the stack and its permit, a baler if the supplied one is not wanted, and two operators. Commissioning takes five to seven days, including a burn-off trial on each section range and a stack test at the design feed rate.
Two operators is the honest number: one at the loader and the zone panel, one at the baler and the yard. A single operator works only while the belt is stopped, because the loader has to be cleared before a bale can be tied and the two positions are eight metres apart.
The first trap is buying this size for a feed that is mostly 3–4 mm profile. Dwell at 12–16 minutes caps throughput near 0.7 t/h on heavy section, and the line will never see its rating; the three-zone tunnel with 14 m of heated length is the correct unit for that mix. The second trap is deleting the spreader or the cooling section to save capital — both are cheap, and both determine whether the output is a premium charge or a smoky one.
Above roughly 1.8 t/h of mixed sheet and profile, the next step is the 3 t/h three-zone line, which carries the same zone philosophy with a longer heated length and a wider belt.
MSK Machinery quotes this tunnel with the zone programme written for the buyer’s actual section mix. Fabrication is by Henan MSK Machinery Co., Ltd. of Xingyang, Zhengzhou, Henan, and the trading entity behind https://sinoqtech.en.alibaba.com/ can be checked against the company registration.
Related pages
MSK network
Aggregates and mining equipment: mskmachinery.com. Export contracts: Sino Qtech Industries.
Manufacturer and compliance facts
Henan MSK Machinery Co., Ltd. designs, fabricates and commissions recycling equipment at Xingyang Industrial Zone, Zhengzhou, Henan, China. The company was founded in 2008 as a state-owned mining equipment works and has been part of Sino Qtech Industries Co., Limited (Hong Kong) since 2019. Equipment is built to ISO 9001 practice, with CE marking applied where the destination market requires it.
References used in this page’s engineering claims: EU WEEE Directive 2012/19/EU · Basel Convention on waste shipments · US DOE — Waste Reduction & Recycling · ISO 9001 quality management
Questions buyers ask before the proposal
Can the tunnel decoat 4 mm profile at full rate?
It will decoat it, but at 12–16 minutes dwell the throughput falls to about 0.7 t/h. The one-tonne rating applies to mixed sheet and thinner profile.
What metal loss should be expected on 4 mm profile?
0.8–1.8 % depending on section. Foil at 0.05 mm sits at the top of the range because it has the highest surface-to-mass ratio and heats fastest.
How often is the mesh belt replaced on 2 shifts?
Every 8–14 months on a two-shift pattern. Thermal cycling, not abrasion, is what cracks it, so a gentle cooling section extends belt life noticeably.